MIL-DTL-46192C(MR)
TABLE I.
Chemical composition, percent (ladle analysis).
__________________________________________________________________
Element
Min.
Max._______
Silicon
-
0.25 1/
Iron
-
0.30 1/
Copper
5.3
6.4
Manganese
0.10
0.50
Magnesium
0.05
0.40
Titanium
0.02
0.10
Zinc
-
0.10
Zirconium
0.10
0.25
Vanadium
0.05
0.15
Others, each
-
0.05
Others, total
-
0.15
Aluminum
Remainder
____________________________________________________________________
1/ The combined silicon and iron content shall not exceed 0.40 percent.
3.5 Stress-corrosion resistance. When stress corrosion testing is specified in
the contract or order (see 6.2), plate 0.75 inch and greater in thickness shall
be resistant to stress corrosion cracking, with 3 out of 3 specimens not showing
evidence of cracking when tested in accordance with 4.7.3.
3.6 Thermal processing. Heat treatment shall conform to the requirements of
AMS 2750 and 2772 and shall be such as to enable the material to meet the
requirements of these specifications.
3.7
Dimensions and tolerances.
3.7.1 Dimensions. Size of plate shall be as specified in the invitation for
bids, contract or order (see 6.2).